How should AISI 316L be drilled correctly?
Drilling AISI 316L means fighting its greatest enemy: work hardening. The fundamental rule is “never stop”. The drill must keep cutting continuously; every hesitation or pause in the hole instantly hardens the material, making further penetration impossible or destructive to the tool. It is essential to use drills with a large point angle (140°) to improve self-centering and reduce axial thrust, and to ensure perfect chip evacuation through high-pressure internal coolant.
Which drills should be used to drill AISI 316L accurately?
Precision requires rigidity and geometry:
- Solid Carbide (VHM): HSS drills deflect too much. Micrograin K15/K20 carbide provides the rigidity required for H7/H8-tolerance holes.
- Coating: A heat-resistant TiAlN or AlCrN coating with low friction is essential to avoid adhesion (BUE).
- Geometry: Drills with a 4-facet grind or web thinning reduce thrust force and improve centering.
Which drilling parameters are recommended for 316L stainless steel?
Parametri consigliati per punte VHM 5xD su 316L:
- Vc: 60-80 m/min. Do not exceed this range to avoid burning the cutting edges.
- Feed (fn): 0.08-0.15 mm/rev, depending on diameter.
- Drilling Cycle: Avoid pecking if possible. If required (holes >3xD without through-coolant), peck only occasionally and never allow the drill to rub on the bottom. The tool should re-enter the hole already under feed.
How can work hardening and overheating be avoided when drilling AISI 316L?
To prevent thermal and structural damage:
- Coolant: Supply 10-12% emulsion internally. The oil reduces friction and the water removes heat.
- Pilot Drill: For deep holes (>8xD), always use a short pilot drill (1-2xD) with the same or a slightly larger point angle (e.g. 142°) to guide entry without vibration.
- Exit Control: Reduce feed by 40% in the last few millimeters before breakthrough to avoid a “cap burr” and chipping of the drill edges.