How can the finish on Grade 5 titanium be improved?
Achieving a mirror-like surface finish (Ra < 0.4 µm) on Grade 5 titanium (Ti-6Al-4V) requires preventing elastic springback and high-frequency vibration. Titanium tends to “grab” the tool; if cutting pressure is not constant, the surface becomes dull and torn. The key is to use finishing cutters with a high flute count (5 or more), high helix angles (45° or more) to maintain continuous contact with the workpiece, and climb milling with the correct finishing allowance (at least 0.1-0.2 mm) so that virgin, non-work-hardened material is cut.
Which end mill should be used to achieve a good surface finish on Grade 5 titanium?
Cutter selection is decisive:
- Number of Flutes: Use 5, 7, or even 9 flutes. More flutes mean smaller scallop spacing at the same table feed.
- Helix Angle: A strong helix (45°-50°) reduces initial impact and provides a soft cutting action.
- Radius: A corner radius not only improves strength but also distributes surface marks better than a sharp corner.
How can tool marks and vibration be reduced when finishing titanium?
Common mistakes to avoid:
- Dwell: Never stop on the surface. A cutting edge rotating without feed creates chatter marks immediately.
- Insufficient Finishing Allowance: If only 0.02 mm is left for finishing, the tool rubs rather than cuts, polishing irregularly and leaving marks.
- Vc: For finishing, Vc can be increased (80-100 m/min) compared with roughing because contact time is short.
Which parameters improve titanium finishing while reducing burrs?
“Zero-burr” parameters:
- Smooth Exit: Program an arc-shaped roll-out to prevent the edge from tearing the final strip of material.
- Sharp Edges: Use new cutters for the final pass. A cutting edge with wear > 0.05 mm dramatically increases burr formation on titanium.